38CrSi steel chemical composition
C |
Si |
Mn |
S |
P |
Cr |
Ni |
Cu |
0.35~0.43 |
1.00~1.30 |
0.30~0.60 |
≤0.035 |
≤0.035 |
1.30~1.60 |
≤0.030 |
≤0.030 |
38CrSi steel mechanical properties
The sample blank dimensions(mm):25
Heat treatment:
The first quenching heating temperature (℃) : 900; Coolant: oil;
The second quenching heating temperature (℃) : tempering heating
Tensile strength σb (MPa):≥960(100)
Yield strength σs (MPa):≥840(85) Elongation δ5 (%):≥12
Reduction of area ψ (%):≥50 Impact energy Akv (J):≥55
Impact toughness values αkv (J/cm2):≥69(7)
Brinell hardness (HBS100/3000) or high temperature tempering, annealing state) : ≦ 255
Delivery status: by heat treatment (normalizing, annealing and high temperature tempering) or heat treatment state delivery, delivery status should be indicated in the contract.
38CrSi steel main features: it is a kind of high intensity, the medium toughness of steel, it is the hardenability of a little well, than 40 cr in oil critical hardening of 25-83.5 mm in diameter; Steel machinability is good, but you have temper brittleness tendency of heat treatment, cold and low deformation plasticity, poor weldability.